Chinese researchers have treated linden wood so that it can be bent and shaped while wet into items such as cutlery, plates, and straws. Upon drying, the material densifies and becomes significantly stronger. The research was published online as an accepted manuscript in the Journal of Bioresources and Bioproducts and focuses on a potential alternative to disposable plastic products.
The team at Nanjing Forestry University builds upon the natural fiber structure of the wood. First, a small portion of the lignin is removed—the substance that binds wood fibers together and makes the wood stiff. Next, cellulose dissolved under vacuum enters the pores. As soon as the wood is placed in water, this cellulose precipitates as a fine network that connects the existing fibers. The added cellulose accounts for approximately 3 percent of the final weight.
Water acts as a temporary plasticizer in the treated wood. The fibers can slide past each other without the material breaking. In the tests, the wet wood could be folded almost in half and shaped into the desired form in molds, whereas untreated linden wood broke when folded.
Almost six times as strong
During drying, the wood cells contract into a compact structure without the use of a press. The density increased from 0,48 to 1,16 grams per cubic centimeter. The tensile strength was approximately 406 megapascals, nearly six times higher than that of untreated linden wood. According to the authors, this value is also well above that of plastics such as polypropylene and nylon. The measurements apply to loading in the direction of the wood grain.
Forming takes place at room temperature, but the entire process involves steps with heating and cooling. The pretreatment lasts half an hour in a bath of sodium hydroxide and sodium sulfite at 99 degrees. To dissolve the cellulose, a mixture of lye and urea cooled to minus 12 degrees is required. The formed pieces then dried for six hours in an oven at 60 degrees.
Straw remains stiff in hot water
Because most of the lignin remains in the wood, the material is more water-resistant than pure cellulose products, according to the researchers. The lignin content dropped from only 27,6 to 24 percent. A straw made of the treated wood was still stiff after three hours in water, whereas a paper straw became soaked within half an hour. The wooden straw also retained its shape after half an hour in 90-degree water. A straw made of the bioplastic PLA deformed under the same conditions.
The wood is not completely waterproof. After 48 hours in water, it had absorbed 54 percent of its weight in moisture. After one hour of immersion, the tensile strength was still approximately 87 megapascals, well over one-fifth of the dry value. Alternately wetting and drying it three times further reduced the strength, to 286 megapascals dry and 47 megapascals wet. According to the authors, this could limit long-term use in fluctuating humidity.
In a burial experiment on the university campus, a wooden straw fell apart into fragments within ninety days. After six months, it had almost completely degraded. A polyethylene straw buried for comparison showed no visible degradation during that period. A life cycle analysis from raw material to factory gate indicates a lower climate impact than that of six common fossil plastics. Transport, use, and waste disposal are excluded from that calculation.
The tests were conducted with four-millimeter-thick planks. With planks thicker than one centimeter, the cellulose solution has difficulty penetrating uniformly everywhere. Differences in lignin content between wood species can also influence the outcome. For scaling up, the scientists mention a simpler process, continuous impregnation, faster drying, and chemical recovery as points of attention.
Source: Li et al., Journal of Bioresources and Bioproducts (2026)